Originally Posted by
John TenEyck
Thanks for the input Hoang. I sprayed 3 - 4 mils. At less than 3 mils and it didn't flow out worth a hoot. At 5+ it looked like a plastic film. So you added GF Extender to get it to flow out well? Ok, I can see how that would help. But how did you get it to dry so quickly? It sure didn't for us. Maybe the temp. was higher and/or the RH lower? And were you satisfied with the hardness? I could scratch it off with my finger nail even a couple of days after spraying. It was incredibly clear, I will say that, even the medium rubbed effect we used.
That's the thing about Enduro Clear Poly; you don't have to add anything to it, or thin it, or even hit a narrow wet mil thickness. It sprays great straight from the can over a pretty wide range of gun conditions, flows out well at both light and heavy coats and dries fast and hard. If you have not yet tried it, I would be very interested in your comments after you do. Hint.
John