I decided to trying spraying both cans of EV II. The old (yellow) stuff had a viscosity of 28 seconds through a #4 Ford cup. The new (white) on was 30 seconds. I used a 1.0 mm needle to spray them.

The new stuff sprayed fine, without defects, and sanded to powder in two hours. After three coats it looked like this:




The old stuff didn't lay down nearly as well and was close to orange peel. Worse, it had bubbles in every coat. This is what it looked like wet after the second coat:




This is what it looked like dry after 3 coats:



I don't know which can represents good EnduroVar II, but the yellow stuff is unusable. The white stuff can't be brushed but sprays well. I'll test it for durability after a few weeks. It will have to be bulletproof for me to consider buying it again, assuming the white stuff is what EnduroVar II is supposed to be.

John